At first Secure a sample of sufficient size that is representative of the material under inspection. Use a fresh portion of the sample for each set of two determinations. Melt the sample slowly until the temperature reaches at least 11°C (20°F) above the expected drop melting point. Place sufficient sample in a flat bottom container to give a sample depth of 12 +- 1 mm. 

Adjust the temperature of the sample to at least 6°C (10°F) (Note 2) above its drop melting point using any general laboratory thermometer for measurement. Chill one of the test thermometer bulbs to approximately 4°C (40°F). 

Wipe dry, and, quickly but carefully, immerse the chilled bulb vertically into the heated sample until it touches the bottom of the container (about 12 mm submerged) and withdraw it immediately. 

Hold the thermometer vertically away from the heat until the surface dulls, and then place it for at least 5 min in water having a temperature of 16 +- 1°C (60 +- 2°F). Prepare another specimen from the same sample using this procedure.

NOTE 2
A dipping temperature of 11°C (20°F) above the congealing point in accordance with Test Method D938 usually will be 6 to 11°C (10 to 20°F) above the actual drop melting point.

Securely fix the thermometers in the test tubes by means of suitable stoppers, such as corks, so that the tip of each thermometer is approximately 15 mm above the bottom of its test tube. Insert the test tubes in the water bath which is at 16 +- 1°C (60 +- 2°F) and adjust the height of the test tubes so that the immersion marks on the thermometers are level with the top surface of the water. 

Raise the temperature of the bath at a rate of approximately 2°C (3°F)/min to 38°C (100°F), then at a rate of approximately 1°C (2°F)/min until the first drop of material leaves each thermometer. Record in each case the temperature at which the first drop falls from the thermometer.

procedure for melting process non petroleum jelly cooling and hardening

Tag : zibro, petromax, petrol, petrolatum cosmétique, huile minérale, petrolium, white petroleum jelly, vaselin jelly, petrolatum jelly, white petrolatum, petroleum jelly, cetearyl alcohol, white petrolatum usp, vasaline, pure petroleum jelly, petrolium, lanolin alcohol, vasline, phenyl trimethicone, petrolium jelly, petroleum gel, fougera white petrolatum usp, petrolatum gauze, petrolatum usp, petrolatum jelly, what is petrolatum, petrolatum msds, petrolatum ointment, petrolatum dressing, white petroleum jelly, petrolatum side effects, white petrolatum jelly, liquid petrolatum, hydrated petrolatum, hydrophilic petrolatum, white petrolatum ointment, petrolatum ingredients, petrolatum white, xeroform petrolatum dressing,

1 comments:

  1. 1xbet korean soccer betting guide | Legalbet
    1xbet korean soccer betting 메리트 카지노 쿠폰 guide – the best betting strategies and the best bookmaker offers. 1XBet korean soccer betting guide septcasino – the best 1xbet betting strategies and

    ReplyDelete